What a CT Grade Actually Means
ISO 8062-3 defines casting tolerance as CT grades from CT1 (tightest) to CT16 (loosest). Two rules trip people up: the CT value is a total tolerance band, not a ± value — halve it to get bilateral tolerance — and the band widens with the nominal dimension, so the same grade is easier on a 20 mm feature than on a 200 mm one.
The table below gives total tolerance bands for the grades most relevant to investment casting. Divide by two for ±.
“Can you cast a bore to ±0.05 mm?” — No foundry can, and the drawing should not ask. As-cast bores land in the CT6–CT8 range with some core shift. If the bore is functional, specify it as-cast with machining allowance and hold ±0.05 mm on the machined feature instead.
Which Process Gets Which Grade
What Loosens Tolerances on Real Parts
CT grades assume reasonable design. Expect the band to drift toward the loose end when:
- The dimension is large. Shrinkage compensation is applied per alloy, and absolute variation grows with size even at constant grade.
- Cores define the feature. Internal passages and bores carry core shift in addition to shell variation; core-printed locations are the least predictable surfaces on the part.
- Walls are thin or sections change abruptly. Differential cooling distorts the casting away from the nominal geometry.
- Cut-off and cooling leave residual stress. Parts can move slightly after gating removal; critical flatness is earned by machining, not by casting.
How to Specify Tolerances So You Get Them
The drawings that produce accurate castings share a pattern, and it costs nothing to adopt:
- Mark a general CT grade on the drawing (e.g., “ISO 8062 – CT6”) instead of putting machining-level ± on every dimension.
- Flag the critical few. Datums and functional features get their own tighter grade or a machining note with stated allowance.
- Give machining allowance where metal is cut. Specify enough stock for the cutter to clean up the cast surface — the CT article in our library covers allowance selection in detail.
- Let the foundry review before tooling. A DFM pass on the model converts tolerance surprises into design changes while they are still free.
“Should every dimension on the drawing be tight?” — No. Tightening a non-critical dimension from CT6 to CT4 buys nothing except cost and yield risk. Spend precision only where the part actually functions: fits, sealing, mounting, and datums.
To Summary
Cast as-cast tolerances in the CT5–CT7 band with silica sol investment casting, CT9–CT11 with water glass, and treat anything tighter than roughly ±0.1 mm as a machined feature with declared allowance. Tolerance is a design conversation, not a supplier boast: mark the grade, flag the critical few, and send us the model — our DFM review will tell you exactly which features land near-net and which need a cutter.