A356 vs A360 vs ADC12: Choosing Among the Three Most-Used Aluminum Die Casting Alloys
Aluminum die casting alloys are specified by a single trade-off repeated across every RFQ: structural performance on one side, fillability and cost on the other. Three grades account for the overwhelming majority of parts ordered worldwide — A356, A360 and the JIS grade ADC12 — and choosing among them is usually decided before the die is even cut.
This guide walks through each of the three aluminum die casting alloys on its own terms: chemistry, heat-treatment response, defect behavior and the applications where each one is genuinely the right answer.
The Line That Splits Aluminum Die Casting Alloys
The first division is not between A356 and A360 or A360 and ADC12 — it is between heat-treatable and non-heat-treatable. A356 is an Al-Si-Mg alloy (roughly 7% silicon, 0.35% magnesium) whose strength comes from the Mg₂Si aging reaction: solution treat, quench and age to T6, and the part can reach 310 MPa tensile with several percent elongation. A360 and ADC12 are Al-Si-Cu alloys (8–12% silicon, 1.5–3.5% copper) whose strength is fixed as-cast; they cannot be solution treated without blistering and overaging, so whatever the die gives is what you keep.
That single fact eliminates candidates faster than any property table. If the part must be T6’d, welded or crash-rated, you are shopping in A356 territory. If it is a thin-wall housing produced at hundreds of thousands per year, the copper-bearing grades win on flow and price.
A356: The Structural Choice
A356 (the wrought-equivalent family EN AC-46000 / AlSi7Mg) is the grade behind wheels, suspension knuckles, steering components and vacuum-assisted structural die castings. Its hypo-eutectic chemistry gives it the lowest iron and oxide inclusion sensitivity of the three, and its heat-treatment response gives design engineers real strength margins.
The costs are equally real. A356 has noticeably poorer fluidity than the near-eutectic grades, so thin walls and long flow paths demand more aggressive — and more expensive — gating and vacuum systems. It is also prone to hot tearing during solidification shrinkage if the die thermal design is careless, and every part carries a T6 furnace pass plus the quench-distortion control that comes with it. Specify A356 when the part is loaded, safety-related or weldable; do not specify it merely because the datasheet numbers look better.
A360: The Workhorse Housing Alloy
A360 sits at nearly eutectic composition — about 9% silicon with 2.5–3.5% copper — which gives it excellent fluidity, low hot-tearing tendency and good pressure-tightness potential in as-cast (F) condition. Typical published as-cast properties run around 240–250 MPa tensile with 3–4% elongation, adequate for the enclosures, gearbox cases, motor housings and small-engine components that consume most of the world’s A360.
Its machine behavior is friendly too: the copper content raises hardness and improves chip breakability relative to purer Al-Si alloys, so drilled and milled sealing faces come out clean. The limits are structural and thermal — A360 softens on sustained heating above roughly 150–200°C as its Cu-rich phases coarsen, and like all high-silicon die-cast alloys it welds poorly. Gas-shielded arc welding of A360 parts generates silicon melt at the joint and porosity that no welder enjoys explaining afterward.
ADC12: The High-Volume Production Grade
ADC12, defined in JIS H5302 and dominant across Asian high-pressure die casting, pushes silicon to roughly 9.6–11.8% with 1.5–3.5% copper and a deliberately generous iron allowance (up to about 1.3%). That last detail is the whole story: higher tolerated iron means less die soldering and longer die life when running secondary or scrap-heavy melts, which is precisely what high-volume consumer and automotive bracket production cares about.
ADC12 fills thin walls beautifully and costs the least per shot of the three aluminum die casting alloys. The trade is ductility and integrity: the coarse intermetallics that come with high Si plus high Fe keep elongation low, heat-treating is off the table, and weldability is effectively zero. For housings, brackets, covers and electronic enclosures it is the volume champion; for anything structural, fatigue-critical or repairable, look up this article’s earlier sections.
Defect Personalities You Must Design Around
Each of the three aluminum die casting alloys fails in its own characteristic way, and a good DFM report treats them differently:
- A356 — hot tears at rigid cores and abrupt section changes; shrinkage porosity in last-to-freeze bosses unless local cooling or overflows are added.
- A360 — entrapped gas porosity when biscuit and overflows are undersized; the alloy flows well, so it faithfully records every turbulence event in the shot.
- ADC12 — low ductility cracking at ejector pins and sharp internal radii; iron-rich intermetallics make it unforgiving of thin, constrained geometry.
Wall thickness, radii, draft and gate location should all be negotiated per grade, not per family — a housing redesigned from ADC12 to A356 without re-running the thermal simulation usually arrives with new defects, not fewer.
Q: Can I switch my drawing from ADC12 to A360 (or vice versa) without re-quoting the tool?
A: Expect to re-validate, not just re-letter the print. The two grades differ in shrinkage, die-soldering tendency and required shot parameters, which shifts gate and overflow design. A grade swap on an existing die is possible but should be treated as a new process qualification with dimensional and X-ray checks on first articles.
Four Questions That Decide
1. Will the part be heat-treated, welded or crash-loaded? Any yes forces A356 — the only heat-treatable grade of the three aluminum die casting alloys, and the only one with meaningful as-cast ductility after T6.
2. How thin and how long is the flow path? Sub-1.5 mm walls with long runs favor A360 or ADC12; A356 will fill them only with vacuum assistance and premium gating.
3. What is the annual volume and scrap policy? At high volume with recycled furnace feed, ADC12’s iron tolerance and price per shot win; at low volume with strict integrity requirements, that same tolerance becomes a liability.
4. Does the part need a machined seal or pressure tightness? A360 machines cleanly and can be sound enough for moderate pressure test; ADC12’s porosity tendency demands generous skin allowance and conservative leak specs.
To Summary
The three grades sort themselves along one axis: A356 buys heat-treatable structure at the price of fluidity and process cost; A360 buys balanced flow, machinability and housing performance in the as-cast condition; ADC12 buys maximum fillability and minimum cost per shot for high-volume non-structural parts. Ask the four questions above before the die design freezes, and the choice among aluminum die casting alloys stops being a datasheet argument and becomes a straightforward trade of strength against flow and price.
About ATM-Casting: ATM-Casting provides die casting and CNC machining services for aluminum housings and structural components, including A356, A360 and ADC12 production with vacuum assistance and full first-article validation. For grade selection, DFM review or quotation on aluminum die casting alloys, contact our engineering team.